From: Self-assembling Fmoc dipeptide hydrogel for in situ 3D cell culturing
Dispersion Medium | Gelling Agent Concentration (mg/ml) | Final Peptide Concentration (wt%) | Hydrogel Assembly Result |
---|---|---|---|
1. PBS 10× | 100 | 0.5 | Unstable |
2. PBS 1× | 100 | 0.5 | Unstable |
3. PBS 1× | 100 | 1.0 | Partial |
4. PBS 1× | 25 | 0.5 | Soft Gel |
5. PBS 1× | 25 | 1.0 | Firm Gel |
6. MEM | 25 | 0.5 | Unstable |